Powder coating additives – I leveling agents, degassing agents, texturing agents, matting agents
来源: | 作者:佚名 | 发布时间 :2025-04-07 | 544 次浏览: | 🔊 Click to read aloud ❚❚ ▶ | Share:

1 Introduction

In addition to binders and pigments, there are also some important substances --- additives that obviously affect the appearance and curing degree of the coating film, which are specially used in powder coatings to make the application performance of polymer binders smoothly produced and added to the powder coating binders. Additives play a very important role in the formulation of powder coatings, so that they become an indispensable part .

The ideal additives should have the following characteristics: solid, preferably crystalline fine powder with a melting point or glass transition temperature of more than 50 degrees; Good stability, easy to store and use; No chemical reaction with resin binder or curing agent; It should be colorless or light-colored, and the coating film cannot be colored; with specific features; 100% active; Where possible, low addition levels can help; It is basically non-irritating and toxic, and meets the relevant environmental safety standards. However, in most cases, many of the most useful additives are in liquid form, so they are often added to the resin or adsorbed on a carrier to make a masterbatch.

 

    2 Leveling agent

Leveling agents have been used for many years and are still developing, and their main role is to prevent the occurrence of coating defects (such as craters, fisheyes, etc.) and to reduce orange peel. At the same time, the use of leveling agents helps to improve the dispersion of pigments and the degassing effect during the curing process, increasing the fluidity and other effects. The good dispersion effect promotes the dispersion effect of the pigment in the system, enhances the color uniformity and reduces the processing time.

Usually when an acrylic polymer additive is "additional" added, the excess leveling agent migrates to the surface of the molten resin (which is generally enhanced by its incompatibility with the coating system), thus compensating for its chemical potential energy in the base surface and body. The side chains of the alkyl groups, on the other hand, tend to escape outwards and reach some stable equilibrium state. Therefore, due to the high concentration of molecular structures arranged in the whole surface, the tension of the whole surface tends to be average. The film formation and flow of the powder coating is controlled by two main parameters: surface tension and melt viscosity, and the surface tension (at a given temperature) is the main driver of flow, and the only flow resistance comes from the melt viscosity of the powder under baking conditions. Therefore, leveling agents can be more accurately defined as surface tension improvers.

 

   Theoretically, there must be two prerequisites for controlling the flow of powder coatings:

(1) High surface tension, but in order to ensure that the substrate can be fully wetted, it should not be higher than the surface tension of the substrate.

(2) The surface tension must be locally uniform at the interface with the air.

 

    Without the use of leveling agent, the powder coating not only has poor fluidity, orange peel is produced, but also the surface of the coating film tends to produce pinholes. Surface defects are not related to the substrate, so they cannot be considered as "substrate wettability" is not good, but is caused by "extremely poor fluidity".

 

    In order to ensure good wetting performance, the leveling agent should be evenly dispersed in the powder system, and good dispersion in the production process is necessary. There is also the possibility of interference with each other, and the sequential production of high surface tension varieties to low surface tension varieties is applied in the actual production arrangement to reduce the occurrence of cross-contamination phenomenon. However, there are still some modified polysiloxanes (such as polyether and polyester modified polysiloxanes) that can improve the leveling of powder coatings without contamination.

 
Generally, leveling agents are viscous liquids, so they are usually added to the resin at a one-time concentration of 5% to 15% or precipitated onto fumed silica at a concentration of 60% to 70% to make a masterbatch. Some high molecular weight thermoplastic polymers are also very effective in preventing cratering in powder coatings, such as polyvinyl butyral used as a leveling agent, because they have a high melting point, so it is difficult to disperse into the resin melt during extrusion, so they are soon replaced by liquid polyacrylic acid.

 

    3 Degassing agent

The most commonly used degassing agent is benzoin, which acts as a solid solvent to make the coating film continuously unfold, and has a long enough time to allow the air to escape from the coating film. People recommend a minimum increase of 0 for benzoin. 2% (according to the total amount of formulation) For white and off-white paints, if over-baking is involved, the addition can not exceed 0.2%, and for black or other dark systems, it can be increased up to 0.8%. , so its use is limited by storage stability; Derivatives of hydrogenated castor oil will also improve the fluidity of the coating film, but reduce the glass transition temperature; a wide variety of polyethylene and polypropylene wax (if they do not have matting function); Mono or diamide wax .

 

    In order to obtain a better degassing effect, it is best to choose a suitable degassing agent according to the processing characteristics of different systems, and the combination of benzoin and other degassing agents will be better.

 

   4 Texturing agent

These products can provide a structural effect to the surface, which is characterized by a uniform surface texture and uniform gloss and color, and some insoluble or incompatible additives are added to control the particle size, melt viscosity, and surface tension of the molten surface, so as to achieve the desired texture effect.

Textured powder coating is a general term and comes in different varieties. Such as sand pattern, wrinkle type, water pattern type, etc., this kind of additives are more special, and the fruit will not be obvious or even make the coating film smooth.

 

    (1) Sand grain

In the early preparation of sand grain powder coatings, a large number of fillers were often added, or the gelling time of the powder was shortened, or a combination of the two, and its disadvantages were self-evident.

(2) Wrinkles

In the wrinkle powder coating, the sudden change of the local surface tension in the powder system will lead to an increase in the degree of disorder and produce depressions, which is one of the most basic principles for us to make wrinkle powder. CAB (acetate butacellulose) is one of its additives. CAB will reduce the surface of the coating film to produce controllable "defects", when the powder is heated, CAB produces a very low surface tension in the molten state, and the surrounding powder forms a surface tension difference to produce depressions.CAB The biggest advantage is that it can be co-extruded with other components of the powder without easy to produce the bottom phenomenon, and the dosage is generally 0. 005 %-0. Between 5%, the paint in the concave point does not completely flow away, so that these shrinkage holes do not extend to the substrate and expose the bottom. The exact amount of dosage depends on the desired effect and the type of powder used. When the CAB dosage is relatively high, the effect will not be obvious or even the coating film will be smoothed.

 

    (3) Dermatostriae

Pattern powder coatings can be made with polymer additives that reduce the fluidity of the coating film or do not melt in the binder, for example, the styrene-maleic anhydride copolymer series (SMA) with a melting point range of 55 to 150 degrees can produce fine lines and coarse lines in epoxy and mixed powders without affecting the mechanical properties, and the recommended dosage is 2%-7% of the total amount of binder.

(4) Water ripples

The additives that produce water ripples or cotton lines can be obtained by a special organoaluminum compound, which can be used to produce water ripples in epoxy, mixed and TGIC systems, in which the organoaluminum compound can be used as a curing agent for epoxy powder alone, with a dosage of 10%-15%, and a matte surface with good mechanical properties can be obtained by complete curing. Adjusting the amount of filler and additive can obtain water ripples of different surface gloss and texture size, and special surface texture structure can also be obtained through appropriate formula adjustment, with a strong three-dimensional feeling.

5 Matting agent

Matting agent is defined as a product specially designed to reduce the gloss of powder coatings, and it does not affect the chemical quantitative relationship of the resin system. However, the viscosity of powder coating is quite large in the curing process due to the absence of solvent, and the migration from low viscosity to solid phase is not easy to occur, and the pigment and filler can not accumulate in large quantities on the surface of the coating film, so the matting of powder coating has certain particularities.

The gloss of powder coatings can be broadly divided into 5 grades: high gloss [ high > 85 %, standard [ standard ] 70 % -85 %, semi -gloss or satin [ semi -gloss or satin ] 40 % -70 % low [ low ] 15 % -40 % and matt [matt] <15 %.The variety of matting in the whole powder coating system accounts for a considerable proportion.Generally speaking, the matting of powder coating can be achieved by the following methods.

(1) Filler addition method (2) Addition of incompatible substances (3) Dry mixing method (4) One-time extrusion method